Guangzhou Kebao insulation products Co., Ltd.
Property |
Requirement |
Test method |
Typical data |
Longitudinal shrinkage |
≤5% |
ASTM D 2671 |
≤3% |
Tensile strength |
≥13.8 MPa |
ASTM D 2671 |
≥19 MPa |
Elongation at break |
≥150% |
ASTM D 2671 |
≥ 250% |
Tensile strength after ageing (232℃,168hrs) |
≥9.7 MPa |
ASTM D 2671 |
≥14 MPa |
Elongation after ageing (200℃,168hrs) |
≥100% |
ASTM D 2671 |
≥ 250% |
Heat shock(260℃,4hrs) |
No crack |
ASTM D 2671 |
No crack |
Low-temperature flexibility(-65℃,4hrs) |
No crack |
ASTM D 2671 |
No crack |
Dielectric voltage withstand |
2500V,60sec, no breakdown |
ASTM D 2671 |
pass |
Volume resistivity |
1015Ω·cm min. |
ASTM D 876 |
≥1016Ω·cm |
Corrosion |
No corrosion |
ASTM D 2671 |
No corrosion |
Flammability |
VW-1 |
UL224 |
pass |
Dielectric constant |
|
|
2.1 |
Friction coefficient |
|
|
0.2-0.3 |
Size
sizes are available upon your request
Property |
Requirement |
Test method |
Typical data |
Longitudinal shrinkage |
≤5% |
ASTM D 2671 |
≤3% |
Tensile strength |
≥13.8 MPa |
ASTM D 2671 |
≥19 MPa |
Elongation at break |
≥150% |
ASTM D 2671 |
≥ 250% |
Tensile strength after ageing (232℃,168hrs) |
≥9.7 MPa |
ASTM D 2671 |
≥14 MPa |
Elongation after ageing (200℃,168hrs) |
≥100% |
ASTM D 2671 |
≥ 250% |
Heat shock(260℃,4hrs) |
No crack |
ASTM D 2671 |
No crack |
Low-temperature flexibility(-65℃,4hrs) |
No crack |
ASTM D 2671 |
No crack |
Dielectric voltage withstand |
2500V,60sec, no breakdown |
ASTM D 2671 |
pass |
Volume resistivity |
1015Ω·cm min. |
ASTM D 876 |
≥1016Ω·cm |
Corrosion |
No corrosion |
ASTM D 2671 |
No corrosion |
Flammability |
VW-1 |
UL224 |
pass |
Dielectric constant |
|
|
2.1 |
Friction coefficient |
|
|
0.2-0.3 |
Size
sizes are available upon your request